Sezvatinoziva tese, kukanda mari kunogadzira iyocastingsnekururama kwechokwadi uye nekupedzisa kwakanaka. Zvisinei, panguva yekugadzirwa kweInvestment casting, kune zvakawanda zvinowanzoitika kukanganisa kukanda. Zvichienderana neruzivo rwedu rweinjiniya uye michina yepamberi, tinogona kuwana nzira yekudzivirira matambudziko akadai nekuongorora zvikonzero. Pazasi, isu tinosuma akati wandei akajairika ekukanda kukanganisa uye zvikonzero zvawo uye nzira dzekudzivirira. Ndinovimba kuti chinyorwa ichi chinobatsira kune vatengi vedu kuti vanzwisise matambudziko uye kune vatinoshanda navo, ongororo iyi inogona kukubatsira kudzivirira izvo zvinogona kukanda hurema.

Undercast uye inotonhora chipingamupinyi
1. Tsanangudzo yedambudziko:
Undercasting kazhinji inoshaya nyama munharaunda mumadziro akaonda ekukanda kana kure nemumhanyi wemukati, uye mupendero wayo wakaumbwa nearc. Iyo inotonhora partition ndeyekuti tambo mbiri dzesimbi yakanyungudutswa haina kusanganiswa zvachose uye kune majoini ari pachena.
2. Chikonzero:
1) Yakaderera simbi yakanyungudutswa ichidira tembiricha uye mold tembiricha
2) Kudurura kumhanya kunononoka kana mumhanyi kugadzika hakuna musoro, kuyerera kwesimbi kwakarebesa
3) Ukobvu hwemadziro ekukanda hwakanyanya kutetepa, uye kuyerera kwesimbi yakanyungudutswa kwakashata
4) Cheka panguva yekudira
3. Matanho ekudzivirira:
1) Wedzera tembiricha yakanyungudutswa yesimbi uye mold tembiricha
2) Wedzera kumhanya kwekudira kana kuwedzera nhamba kana nzvimbo yemumhanyi wemukati kuderedza kuyerera kwesimbi yakanyungudutswa.
3) Wedzera kudzvinyirirwa kwemusoro wekudururira kusimuka kudzivirira kuchekwa-kubviswa panguva yekudira

Shrinkage
1. Tsanangudzo yedambudziko:
Inogona kuwanikwa chete ne X-ray kuongorora. Iyo yepamusoro shrinkage inogona kuwanikwa ne fluorescence kana staining inspection. Muzviitiko zvakakomba, inogona kuwanikwa mushure mekuputika kwejecha.
2. Chikonzero:
1) Chimiro chekukanda hachina musoro, uye nzvimbo dzinopisa dzakanyanya kana kuti dzakakura
2) Kupisa kwesimba rekudururira kudiki, izvo zvinotadza kuumba sequential solidification, kana musoro wekumanikidza idiki, izvo zvinoderedza simba rekudya.
3) Iyo tembiricha yekuumbwa yakadzikira, mwero wekutonhora unokurumidza, uye nzira yekudyisa yakavharwa
3. Matanho ekudzivirira:
1) Kuvandudza maitiro ekukanda uye kuderedza nzvimbo dzinopisa
2) Isa inosimudza zvine musoro, kana kuwedzera mbabvu yekudyisa inogona kubviswa nenzira dzekugadzirisa, wedzera kudzvanywa musoro, kuitira kutiInvestment castingsinogona kusimbiswa sequentially pasi pechiito cheimwe musoro wekumanikidza
3) Wedzera zvakafanira tembiricha yekudurura uye tembiricha yekuumbwa kuti udzikise kutonhora

Hot crack
1. Tsanangudzo yedambudziko:
Irregular intergranular cracks inogadzirwa pamusoro pepamusoro kana mukati, uye pamusoro pacho pane oxidized. Inogona kuonekwa mushure mekuchenesa jecha rakasimba, uye kungogadzirisa zvinyoro kana kuongorora kwekupinda kunogona kuwanikwa.
2. Zvikonzero:
1) Iyo ine hukama nekuumbwa kweiyo alloy, zviri mukati kabhoni nesilicon zvakakwirira, tembiricha yemhando yemvura-yakasimba chikamu yakakura, uye kupisa kupisa kuri nyore.
2) Yakaderera mold tembiricha, kutadza kudzoka uye kukurumidza kutonhora rate
3) Ukobvu hwekukanda hunosiyana zvakanyanya, uye shanduko fillet idiki kwazvo
3. Matanho ekudzivirira:
1) Kune alloys kana masimbi anowanzo kuputika kupisa, kabhoni nesilicon zvemukati zvinofanirwa kudzorwa zvakanyanya sezvinobvira kune yepakati uye yakaderera miganho.
2) Wedzera tembiricha yekuumbwa panguva yekudururira, deredza kutonhora kwekukanda, kana kuderedza simba regoko rekuumbwa.
3) Wedzera anti-kutsemuka mbabvu pamajoini ehukobvu hwekukanda, kana kuwedzera mafiritsi ekuchinja.

Cold Crack
Zita uye Hunhu:
Pane zvinoramba zvichipinda mutsemu pakukanda. Nzvimbo inopenya kana nzvimbo ine oxidized zvishoma inoonekwa pakutyoka.
Zvinokonzera
1. Munguva yekutonhora kwekukanda, shrinkage inodziviswa, zvichiita kuti kupisa kuwedzere uye kushanduka kwechikamu kushungurudza, uye izvi zvinoshungurudza zvinopfuura simba rezvinyorwa muhutano hunoputika uye hunokonzera kuputsika.
2. Muchigadziro chekuchenesa shell, kucheka gedhi, riser kana panguva yekugadzirisa, kukanda nekusarira kunetseka kunoiswa pasi pesimba rekunze kukonzera kuputsika.
Kudzivirira Nzira
1. Wedzera mbabvu dzakaomesesa pamitsipa inotonhora kuti uvandudze kudzoka kwechimiro, nokudaro kuderedza kushomeka kwekudzivirira uye kukanda kushushikana.
2. Mumashure ekukanda maitiro, dzivisa kukanganiswa kwakanyanya pakati pekukanda.

Blowhole
Zita uye Hunhu
Kune maburi akajeka kana asingaoneki ane mukati wakatsetseka pamusoro pekukanda.
Zvinokonzera
1. Kusakwana kwemhepo kupinza kwegomba re mold, izvo zvinoita kuti inyanyononoka kuti gasi riri mugomba ribudiswe panguva yekudira.
2. Kusakwana kupfurwa kwechimiro chegoko, zvichikonzera kusakwana kubviswa kwezvimedu zvekuumbwa uye zvinhu zvinogadzira gasi muhombodo.
3. The metal liquid gas content yakanyanyisa, zvichiita kuti deoxidation yakaipa.
4. Kugadziriswa kwegadziriro yekudurura hakuna musoro, zvichiita kuti gasi remunhu ribatanidzwe mukudurura.
Kudzivirira Nzira
1. Kuvandudza kupinza kwemhepo yegoko uye wedzera mavhavha kana zvichidikanwa.
2. Goko rakazara.
3. Kuvandudza deoxidation nzira.
4. Kuvandudza gating system.

investment casting defect
kukandira kuremara-5

Kukandira Pitting
Zita uye Hunhu
Pane gomba rakakora-rakafanana nemakomba pamusoro pekukanda.
Zvinokonzera
1. Apo ethyl silicate inoshandiswa sebinder, iyo isina kukwana hydrolyzate iri mukugadzira, iyo indoor humidity humidity yakanyanya kuderera, kuitira kuti hydrolyzate irege kuwedzera hydrolyzed, uye "white frost" inonaya mushure mekugocha.
2. Kana girazi remvura richishandiswa sebhainda, munyu wakasara mugoko remuforoma unopindirana nesimbi yakanyungudutswa kuita gomba.
3. Simbi yakanyungudutswa haina kusvibiswa kana kuti slag haina kucheneswa panguva yekubata.
Nzira dzekudzivirira:
1. Paunenge uchishandisa ethyl silicate sebhainda, zvakakodzera wedzera huwandu hwemvura yakawedzerwa uye kuwedzera hunyoro hunoenderana nepende studio kuderedza kusara kusina kukwana hydrolysates.
2. Paunenge uchishandisa girazi remvura sebhainda, chenesa goko nemvura ine acidified mushure mekudonha.
3. Shandura iyo yekuputira pamusoro kune silica sol sebhainda.
4. Panguva yekunyunguduka, simbisa deoxidation uye kubvisa slag.

Kukanda Subcutaneous Pinhole
Zita uye Hunhu
Mushure mekunge pamusoro pekukanda kwakwenenzverwa, madiki matema anooneka. Ichi chiitiko chinowanzoitika mukatinickel-chromium tsvina isina tsvinal.
Zvinokonzera:
1. Zvinhu zvakanyanyoshandiswa zvakare zvinoshandiswa panguva yesimbi yakanyungudutswa, kana kuti iyo yakagadziridzwa haina kubatwa zvakanaka.
2. Panguva yekunyunguduka, simbi yakanyungudutswa yakasvibiswa kana kuti simbi yakanyungudutswa inotora gasi, zvichiita kuti kusakwana kwe deoxidation.
3. Kusachena kwemukati wegoko rakanyanyisa, kana chisungo chekubatanidza nesimbi yakanyungudutswa zvine maitiro emakemikari.4. Kusanzwisisika kwekugadzirisa gating system.

Nzira dzekudzivirira:
1. Kudzora kana kuderedza huwandu hwezvinhu zvakadzokororwa, uye zvinhu zvakagadziriswa zvinoda kushandiswa mushure mekuputika kwejecha kana kuputika kwepfuti.
2. Nyatsodzora maitiro ekunyungudutsa uye kusimbisa deoxidation.
3. Shandisa fused corundum, zircon sand uye silica sol kana ethyl silicate paint.
4. Edza kushandisa jekiseni repasi pakudira uye kuwedzera maburi ekubuda nawo.

Sticky Sand
Zita uye Hunhu
Pane jecha rinonamira padhuze nemumhanyi kana mukati mekukanda, uye kune maburi akasimudzwa kana makomba mushure mekuputika kwejecha.
Zvinokonzera
1. Kusvibiswa kwehupfu hwehupfu hwehupfu hunoshandiswa muhuputi hwepamusoro hwakanyanya kukwirira, uye izvi zvinosvibisa zvinopindirana nesimbi yakanyungudutswa kuti iite eutectic yakaderera yakanyunguduka.
2. Tembiricha yekudurura yakanyanya, kunyanya mamakisi esimbi ane Al, Ti nezvimwe zvinhu, izvo zvinokonzeresa kuita kwemakemikari pakati pesimbi yakanyungudutswa nesilika.
3. Kugadziriswa kwegating system hakuna musoro, uye yakawanda yesimbi yakanyungudutswa inoyerera kuburikidza nemumhanyi wemukati, zvichiita kuti kupisa kwenzvimbo.
Kudzivirira Nzira
1. Shandisa jade resimbi yakasanganiswa kana jecha rezikoni panzvimbo pejecha resilica, uye edza kusashandisa girazi remvura sebhainda.
2. Kudzikisa zvakakodzera tembiricha yekudira.
3. Wedzera mumhanyi wemukati kuti ugadzirise kuenzana kwekupisa uye kuderedza kupisa kwenzvimbo.

Dilatant
Zita uye Hunhu
Kuzvimba kwepanzvimbo pane yakakura ndege yekukanda, chiitiko ichi chinonyanya kuoneka kana uchishandisa girazi remvura sebhainda.
Zvinokonzera
1. Chimiro chekukanda hachina musoro uye nzvimbo yendege yakakura kwazvo.
2. Iyo shell ine simba rakaderera pakupisa kwepamusoro uye haigoni kumira kumanikidzwa kwesimbi yakanyungudutswa.
Kudzivirira Nzira
1. Kuvandudza chimiro, wedzera maitiro mbabvu kana kugadzirisa maburi mundege.
2. Paunenge uchigadzira ganda, shandisa shell zvinhu zvine tsvina shoma uye yakakwirira refractoriness, kana kuwedzera kukora kweganda.

Slag
Zita uye Hunhu
Iko kune slag kana imwe marara mukati kana pamusoro pekukanda. Internal inclusions inoda kuonekwa ne X-ray kana magnetic inspection.
Zvinokonzera
1. Iyo slag zvinhu zvakanyanya kutetepa uye haina kucheneswa isati yarova.
2. Tsvina pamudziyo wekutepfenyura wecrucible haina kucheneswa isati yarova uye yakaunzwa musimbi yakanyungudutswa.
3. Paunenge uchikanda, kuchengetwa kwe slag hakuna kunaka, uye slag inopinda mugomba nesimbi yakanyungudutswa.
Kudzivirira Nzira
1. Gadzirisa kuumbwa kwezvinhu zve slag usati watora kuti uwedzere viscosity yezvinhu zve slag uye kuita kuti zvive nyore kubvisa slag.
2. Chenesa marara mumudziyo wemberi wesimbi kudzivirira kuunza tsvina musimbi yakanyungudutswa muladhi.
3. Asati akanda, iyo yakanyungudutswacast teelinofanira kunyatsoiswa sedated kuti ifambise slag inoyangarara.
4. Tora teapot yekudira ladle ine slag stopper kana ceramic sefa.

Decarburization
Zita nemaitiro
Iyo kabhoni yemukati yekumusoro layer yekukanda yakaderera pane iyo yematrix.
Zvinokonzera
1. Panguva yekukanda, kutonhora kwesimbi yakanyungudutswa uye mold yakakwirira, uye kusimba kwekukanda kunononoka.
2. Kudzika kwe decarburization layer kune hukama nemhepo yenzvimbo inotonhorera yekukanda. Iyo yakanyanya kuwanda kweiyo oxidizing mhepo, iyo yakanyanya kuoma iyo decarburization.
Kudzivirira Nzira
1. Deredzai zvakakodzera tembiricha yekukanda uye tembiricha yekuumbwa kuti ikurumidze kutonhora.
2. Ita zvekugadzira mhepo inoderedza yakapoteredza mold, zvakadai sekuwedzera barium carbonate uye charcoal powder kune mold.